The plausibility check, in one division
A cell’s energy is its nominal voltage times its capacity. Divided by its mass, that gives its specific energy, in watt-hours per kilogram. That number is bounded by chemistry, and no listing can exceed it.
Start from a real 18650, the one in our catalogue: 3.5 Ah at 3.6 V nominal, 48 g. That is 12.6 Wh in 48 grams, or 263 Wh/kg. Which is already at the top of what commercial lithium-ion chemistry can do today.
Now apply the same division to the capacities advertised on marketplaces, at equal mass, since an 18650 is always 18 × 65 mm and always weighs around 48 g.
- Claimed 5,000 mAh: 18 Wh in 48 g, that is 375 Wh/kg — 1.4 times a real cell.
- Claimed 9,900 mAh: 35.6 Wh, that is 743 Wh/kg — 2.8 times a real cell.
- Claimed 12,000 mAh: 43.2 Wh, that is 900 Wh/kg — 3.4 times a real cell.
There is no commercial lithium-ion cell at 743 Wh/kg. Laboratories announce prototypes well below that. A 9,900 mAh listing therefore does not describe a bargain: it describes a lie, and most often a 1,200 to 2,000 mAh cell in a fresh wrapper.
Remember the ceiling rather than the arithmetic: above roughly 300 Wh/kg, in a commercial cylindrical cell, the listing is false. An 18650 over 3,600 mAh, a 21700 over 5,500 mAh: that is the line beyond which you need proof.
Why these cells are dangerous, not merely disappointing
An inflated capacity is not a commercial annoyance. It falsifies everything that comes after.
You size your pack on the advertised capacity. You set your BMS to a current proportional to that capacity. The cell, meanwhile, delivers a third of what is written: it therefore works at three times the intended relative current, heats three times as much, and ages within months.
Worse: the cells of an inflated batch are never matched. The capacity spread between them is enormous, and we have shown elsewhere that a single weak cell drags down a whole pack. With ten mismatched cells, the pack is unmanageable from the first cycle.
The seven checks to run on delivery
On a batch that passes the plausibility check, here is what to verify before soldering anything. None of these needs rare equipment.
- The mass, on a kitchen scale. A cell clearly lighter than its neighbours is hollow, in the literal sense.
- The open-circuit voltage, with a multimeter. A healthy batch arrives within a few tens of millivolts of itself. A cell 0.5 V out has a problem, and a cell below 2 V in LFP is to be set aside.
- The look of the wrapper. Fresh heat-shrink on a supposedly new cell is a signal: people only re-wrap what they want to hide.
- The poles. A weld mark, a scarred or slightly dished pole means the cell has already been built into a pack.
- The markings. A legible manufacturer reference, consistent from cell to cell across the batch, and a date. Ink marking that rubs off with a finger is not marking.
- Swelling, by standing the cell on a flat surface. A prismatic that does not bear on its whole face is scrap, not pack material.
- Internal resistance, if you have a tester. It is the most telling check of all: two cells of the same claimed capacity but very different resistance will never work together.
Where these cells come from, and why
Inflated capacities do not appear from nowhere. They follow three patterns, and recognising them keeps you from going back.
- The re-wrapped cell. A used cell, pulled from a laptop or scooter pack, re-wrapped with an invented label. It is the most frequent case, and the mass check sometimes misses it: the cell really is an 18650, it is simply old.
- The phantom brand. A name that resembles a known manufacturer, one letter off. No serious manufacturer sells under ten different names.
- The "downgraded" batch sold as new. Genuinely new cells, but rejected by the manufacturer for a capacity or resistance defect. They work, and they will not hold the cycles claimed.
In all three cases the question to put to the seller is the same: what is the exact manufacturer reference, and do you have a test report for the batch? An evasive answer is an answer.
The only check that really settles it
The seven above rule out the crude cases. The only one that genuinely measures is a full cycle: charge fully, discharge at a known current, count the amp-hours that come out.
It is slow — several hours per cell — and that is why it is done by sampling a batch, not cell by cell. It is also why test reports have value: they save you from redoing that work.
Every pack we assemble leaves with its own: measured capacity, each cell’s voltage, internal resistance. We quote no figure we have not measured, and the values for the batch in stock come with the quote.
If you already have a doubtful batch in hand, do not build it "to see". Test three cells at random: if the real capacity is more than ten per cent off the claim, treat the whole batch as unknown.